This paper aim to this study are fiberglass transverse reinforced GFRP and carbon FibArmTaptape and reinforced concrete bending beams and were collected 3 RIENFORCED CONCRETE BEAMS In carrying out this work, experimental methods were used to study the mechanical properties of composite materials, bearing capacity, crack resistance, and deformability of the reinforced concrete girder. Externally reinforced concrete beams with GFRP slabs were tested to failure using a two-point symmetric static loading system where two sets of beams were poured for the pilot test program and no fibers were added to the first beam to be compared with other fiber-armed beams and To obtain some physical properties of the fiber strips as the maximum tensile stress they can withstand, and its modulus of elasticity.
Only a few years ago, the construction market began using FRP for structural reinforcement, generally with other building materials such as wood, steel, and concrete. FRPS exhibits many improved properties, such as high strength-to-weight ratio, high stiffness-weight ratio, design flexibility, non-corrosion, high fatigue strength, and ease of application. The use of FRP sheets or panels glued to concrete beams has been studied by many researchers [1] Adhesive fibre-reinforced polymer reinforcement has been established as an effective method applicable to many types of concrete structures such as columns, beams, slabs and walls. Since FRP materials are non-corrosive, non-magnetic and resistant to various types of chemicals, they are increasingly used in the external reinforcement of existing concrete structures. From the previous studies performed, it was shown that externally bonded glass fiber reinforced polymers (GFRP) can be used to enhance the bending, shearing and torsional ability of RC beams [2]
Concrete structures are exposed to damage as a result of some natural disasters such as earthquakes and the floor, or an error occurred during the design, or a defect in the implementation, such as a lack of armament [3]
Some concrete members are not sufficient to withstand the stresses to which they are exposed, or the occurrence of Decrease in reinforcing area as a result of corrosion and rust over time, or a change in function and The source, which carries more service loads for its members than those taken into account during the design Initially, all these things make the establishment unable to perform the function for which it was established Destroying these organs and re-establishing them is a process It is uneconomical in terms of the high cost and the great time and effort to accomplish this Engineers Repairing and restoring these organs is the most appropriate idea for their rehabilitation and treatment [4]
In the past, there were multiple ways in which structures were strengthened Concrete as adding new beams or structural members to the structure, or strengthening the beams by means Mechanical, such as connecting it externally with steel ropes with high tensile strength, but in the early sixties [5-7]
A new technology has appeared in strengthening concrete beams, which is the outer covering using laminate Iron, and effectively this technique achieved a good achievement in terms of increasing the durability and the stiffness of the beams, but There were many problems associated with this technique, such as the heavy weight of the plate, its large thickness, and the difficulty of Loading, lifting, and the need for special machines and equipment during implementation, as well as the problem of rust and corrosion Iron metal suffers when exposed to harsh weather conditions [8-10]
Fiber Reinforced Polymer (FRP) composite can be defined as a type of plastic that has been fiber reinforced and produces a class of materials that fall under a category referred to as composite materials [11]
In general, composite materials are made by scattering molecules of one or more substances into another, which form a continuous network around them [12]
These materials have a high strength-to-density ratio, great wear resistance and appropriate electrical, magnetic and thermal properties However, it is brittle and brittle and its mechanical properties may be affected by loading rate, temperature and environmental conditions [13]
The choice of fiber type mainly controls the properties of the composite materials. Carbon, glass and aramid are the three main types of fibers that are used in construction [14] The final compound is often named by the name of the reinforcing fibers used, for example, CFRP is the carbon fiber reinforced polymer. The most important characteristics that differentiate the types of fibers are stiffness and tensile stress [15]
Fiberglass is mainly made by mixing silica sand, limestone, folic acid and other minor components. Heat the mixture until it melts at about 1260°C.
The molten glass is then allowed to flow through the tiny holes in the platinum plate forming filaments. The glass filaments are cooled and assembled. The fibers are pulled to increase their directional strength. The fibers are then spun into various shapes for use in composites.
Glass-produced fibers are the predominant reinforcement for reinforced polymer composites due to their great dielectric properties, low susceptibility to moisture and high mechanical properties [16]
Glass is generally a well-resistant fiber but weighs more than carbon or aramid, and glass fibers have excellent properties equal to or better than iron in certain applications.
Carbon fibers have a high modulus of elasticity, 200-800 GPa and the final elongation is 0.3-2.5% where lower elongation corresponds to higher hardness and vice versa.
Carbon fiber does not absorb water and is resistant to many chemical solutions. Carbon fiber has excellent fatigue or wear resistance, does not corrode and does not show any creep or sagging [17]
3 RIENFORCED CONCRETE BEAMS were collected and this paper aims at GFRP fiberglass transverse girder, carbon FibArmT tape and reinforced concrete curved girders.
In carrying out this work, experimental methods were used to study the mechanical properties of composite materials, bearing capacity, crack resistance, and deformability of the reinforced concrete girder.
Externally reinforced concrete beams with GFRP slabs were tested to failure using a two-point symmetric static loading system where two sets of beams were poured for the pilot test program and no fibers were added to the first beam to be compared with other fiber-armed beams
To obtain some physical properties of the fiber strips as the maximum tensile stress they can withstand, and its modulus of elasticity.
Table 1- Width of Crack Opening B1
| No. of loading stage | Load, Q, kN | Bending moment, МEd kNm | Width of crack opening | ||||||
| №1 | №2 | №3 | №4 | №5 | №6 | №7 | |||
| 6 | 0.01 | 0.01 | 0.02 | 0.03 | 0.02 | ||||
| 8 | 0.02 | 0.02 | 0.02 | 0.03 | 0.03 | ||||
| 10 | 0.03 | 0.03 | 0.03 | 0.04 | 0.04 | 0.03 | 0.02 | ||
| 12 | 0.04 | 0.04 | 0.03 | 0.04 | 0.06 | 0.03 | 0.03 | ||
| 14 | 0.04 | 0.05 | 0.03 | 0.04 | 0.10 | 0.04 | 0.04 | ||






Table 2- Result of B1
No. of loading stage | Load, Q,kN | Bending moment, МEd кНм | Tensor T1 of concrete | Tensor T2 of reinforcement | deflectometer readinds | The value of the deflection | ||||
indication | Relative deformation of concrete, ‰ | indication | Relative deformation of the reinforcement % | П1, mm | П2, mm | П3, mm | ||||
| 1 | 0 | -0.00 | 0.00 | -0.00 | 0.00 | |||||
| 2 | 2 | -0.01 | 0.43 | -0.04 | 0.455 | |||||
| 3 | 4 | -0.02 | 0.71 | -0.04 | 0.74 | |||||
| 4 | 6 | -0.02 | 1.02 | -0.04 | 1.05 | |||||
| 5 | 8 | -0.03 | 1.16 | -0.04 | 1.195 | |||||
| 6 | 10 | -0.03 | 1.44 | -0.04 | 1.475 | |||||
| 7 | 12 | -0.03 | 1.83 | -0.04 | 1.865 | |||||
| 8 | 14 | -0.03 | 2.21 | -0.05 | 2.25 | |||||
Max q= 17

Figure 1: Development of Deflection under Loading of the Beam B1
Table 3- Width of Crack Opening B2
| No. of loading stage | Load, Q, kN | Bending moment, МEd kNm | Width of crack opening | |||
| №1 | №2 | №3 | №4 | |||
| 1 | 4 | 0.03 | 0.03 | 0.01 | ||
| 2 | 6 | 0.04 | 0.04 | 0.01 | ||
| 3 | 8 | 0.05 | 0.05 | 0.03 | ||
| 4 | 10 | 0.07 | 0.06 | 0.04 | ||
| 5 | 12 | 0.09 | 0.08 | 0.05 | 0.02 | |
| 6 | 14 | 0.10 | 0.10 | 0.06 | 0.04 | |
| 7 | 16 | 0.11 | 0.11 | 0.07 | 0.05 | |
| 8 | 18 | 0.12 | 0.12 | 0.08 | 0.06 | |
| 9 | 20 | 0.14 | 0.12 | 0.09 | 0.08 | |
| 10 | 22 | 0.15 | 0.14 | 0.10 | 0.09 | |




Q max =24
Table 4- Result of B2
No. of loading stage | Load, Q,kN | Bending moment, МEd кНм | Tensor T1 of concrete | Tensor T2 of reinforcement | deflectometer readinds | The value of the deflection | ||||
indication | Relative deformation of concrete, ‰ | indication | Relative deformation of the reinforcement % | П1, mm | П2, mm | П3, mm | ||||
| 1 | 0 | -0.00 | 0.00 | -0.00 | 0.00 | |||||
| 2 | 2 | -0.00 | 0.28 | -0.02 | 0.29 | |||||
| 3 | 4 | -0.00 | 0.54 | -0.02 | 0.55 | |||||
| 4 | 6 | -0.00 | 0.89 | -0.00 | 0.89 | |||||
| 5 | 8 | -0.01 | 1.16 | -0.00 | 1.165 | |||||
| 6 | 10 | -0.01 | 1.42 | -0.03 | 1.44 | |||||
| 7 | 12 | -0.01 | 1.71 | -0.03 | 1.73 | |||||
| 8 | 14 | -0.02 | 2.00 | -0.03 | 2.025 | |||||
| 9 | 16 | -0.02 | 2.39 | -0.03 | 2.415 | |||||
| 10 | 18 | -0.02 | 2.96 | -0.08 | 3.01 | |||||
| 11 | 20 | -0.02 | 3.35 | -0.07 | 3.395 | |||||
| 12 | 22 | -0.05 | 3.94 | -0.05 | 3.99 | |||||

Figure 2: Development 0f Deflection under Loading of the Beam B2
Table 5- Test of a Reinforced Concrete Beam with Destruction along a Section Inclined to the Longitudinal Axis B3
| No. of loading stage | Load, Q, kN | Bending moment, МEd kNm | Width of crack opening | ||||||
| №1 | №2 | №3 | №4 | №5 | №6 | №7 | |||
| 1 | 4 | 0.01 | 0.01 | ||||||
| 2 | 6 | 0.02 | 0.02 | ||||||
| 3 | 8 | 0.04 | 0.03 | 0.01 | |||||
| 4 | 10 | 0.05 | 0.04 | 0.01 | 0.01 | ||||
| 5 | 12 | 0.07 | 0.05 | 0.02 | 0.03 | ||||
| 6 | 14 | 0.07 | 0.05 | 0.03 | 0.04 | 0.01 | |||
| 7 | 16 | 0.08 | 0.05 | 0.04 | 0.04 | 0.03 | |||
| 8 | 18 | 0.09 | 0.07 | 0.04 | 0.04 | 0.04 | |||
| 9 | 20 | 0.12 | 0.10 | 0.04 | 0.04 | 0.04 | |||
| 10 | 22 | 0.14 | 0.13 | 0.05 | 0.04 | 0.06 | 0.01 | ||
| 11 | 24 | 0.16 | 0.14 | 0.05 | 0.04 | 0.08 | 0.01 | ||
| 12 | 26 | 0.18 | 0.16 | 0.05 | 0.04 | 0.08 | 0.03 | ||
| 13 | 28 | 0.18 | 0.16 | 0.05 | 0.04 | 0.08 | 0.05 | ||







Q max= 28.3
Table 6- Result of B3
No. of loading stage | Load, Q,kN | Bending moment, МEd кНм | Tensor T1 of concrete | Tensor T2 of reinforcement | deflectometer readinds | The value of the deflection | ||||
indication | Relative deformation of concrete, ‰ | indication | Relative deformation of the reinforcement % | П1, mm | П2, mm | П3, mm | ||||
| 1 | 0 | -0.00 | 0.00 | -0.00 | 0.00 | |||||
| 2 | 2 | -0.00 | 0.26 | -0.05 | 0.285 | |||||
| 3 | 4 | -0.01 | 0.49 | -0.06 | 0.525 | |||||
| 4 | 6 | -0.01 | 0.89 | -0.06 | 0.925 | |||||
| 5 | 8 | -0.04 | 1.22 | -0.03 | 1.255 | |||||
| 6 | 10 | -0.06 | 1.5 | -0.03 | 1.545 | |||||
| 7 | 12 | -0.08 | 1.87 | -0.03 | 1.925 | |||||
| 8 | 14 | -0.09 | 2.23 | -0.05 | 2.30 | |||||
| 9 | 16 | -0.11 | 2.6 | -0.09 | 2.70 | |||||
| 10 | 18 | -0.14 | 3.04 | -0.12 | 3.17 | |||||
| 11 | 20 | -0.14 | 3.18 | -0.13 | 3.315 | |||||
| 12 | 22 | -0.15 | 3.19 | -0.15 | 3.34 | |||||
| 13 | 24 | -0.15 | 3.19 | -0.16 | 3.345 | |||||
| 14 | 26 | -0.07 | 3.21 | -0.74 | 3.615 | |||||
| 15 | 28 | -0.10 | 3.22 | -0.69 | 3.615 | |||||

Figure 3: Development of Deflection Under Loading Of The Beam 3


Figure 4: Development of Deflection under Loading of 3 Beams
3 REINFORCED CONCRETE BEAMS were collected and this paper aims at GFRP fiberglass transverse girder, carbon Fiber tape and reinforced concrete curved girders where a comparison was made between the first beam with the second and third beam, and several factors were noted, namely, that the highest amount of strength, which is represented in the first beam, is 17 kn. As for the second beam, we note that the strength increased and became 24 kn, as for the last beam, which is also armed with fibers where the force was 28.3kn
Because there are a wide range of combinations between different types of tissue fibers, the strength of the fiber-reinforced polymer varies greatly. The range starts somewhere above 2000 MPa up to about 6000 MPa compared to the more modest range of iron carbon which ranges from 420 MPa to 790 MPa according to ASTM A615-20
Although many FRP producers do not disclose prices for their products, historically fiberglass, regardless of product - is 1 to 1.5 times more expensive than its counterpart made of other materials, for example in steel. What you get from that is a product that will last longer because the product life cycle is much longer.
Engineers and builders need to reinforce concrete structures with materials that can withstand harsh environmental conditions. Fiber reinforcing bars are commercially valuable mainly because they are resistant to corrosive agents and do not leave concrete rust or weaken. GFRP or glass fiber reinforced polymer is one form of FRP. Advanced composite materials such as FRP were approved by the United States and Canada for structural applications in the late 1990s. Sensitive concrete structures such as seawalls, dams and power stations must be reinforced with corrosion resistant steel reinforcement. Therefore, fiberglass reinforcement material is the ideal product for sensitive concrete infrastructures.
Glass fiber reinforced polymer is one of the high value-added construction products and the fact that GFRP is a cost effective building material with the full potential to extend the life of public structures where corrosion can have a huge economic and environmental impact With the rise in corrosion due to global warming, the material gained Fiberglass reinforcement is very popular. In the future, these advanced composite materials will show their strength and properties more clearly.
Because there are a wide range of combinations between different types of tissue fibers, the strength of the fiber-reinforced polymer varies greatly. The range starts somewhere above 2000 MPa up to about 6000 MPa compared to the more modest range of iron carbon which ranges from 420 MPa to 790 MPa according to ASTM A615-20
FRP materials are generally more sensitive than steel reinforcing bars to high temperatures, the type of reinforcement affects the fire resistance of FRP concrete elements; May have lower fire resistance compared to steel reinforced elements of equivalent ambient temperature capacity [1]
The authors declare that they have no conflict of interest
No funding sources.
The study was approved by the University of Grodno, Belarus
ACI Committee 440. (1996). State-of-the-art report on fiber reinforced plastic (FRP) reinforcement for concrete structures. American Concrete Institute. Farmington Hills, Mich, 65.
Saadatmanesh, H., & Ehsani, M. R. (1991). RC beams strengthened with GFRP plates. I: Experimental study. Journal of structural engineering, 117(11), 3417-3433.
Sharif, A., Al-Sulaimani, G. J., Basunbul, I. A., Baluch, M. H., & Ghaleb, B. N. (1994). Strengthening of initially loaded reinforced concrete beams using FRP plates. Structural Journal, 91(2), 160-168.
Alfarabi, S., Al-Sulaimani, G., Basunbul, I., Baluch, M., & Ghaleb, B. (1994). Shear Repair for Reinforced Concrete by Fiberglass Plate Bonding, ACI Structural Journal, 91(3), 458-465.
Malek, A. M., Saadatmanesh, H., & Ehsani, M. R. (1998). Prediction of failure load of R/C beams strengthened with FRP plate due to stress concentration at the plate end. ACI structural Journal, 95(1), 142-152.
He, J. H., Pilakoutas, K., & Waldron, P. (1997, October). Strengthening of reinforced concrete beams with CFRP plates. In Proceedings of the Third International Symposium on Nonmetallic (FRP) Reinforcement for Concrete Structures (pp. 343-350).
Takahashi, Y., Sato, Y., Ueda, T., Maeda, T., & Kobayashi, A. (1997). Flexural Behavior of RC Beams with Externally Bonded Carbon Fiber Sheet, Proceedings of the Third International Symposium on Nonmetallic (FRP) Reinforcement for Concrete Structures, Sapporo, Japan, 327-334.
Swamy, N., Mukhopadhyaya, P., & Lynsdale, C. (1997). Ductility Consideration in Using GFRP sheets to strengthen and Upgrade structures. In Proceedings of the Third International Symposium on Nonmetallic (FRP) Reinforcement for Concrete Structures (pp. 637-644).
Grace, N. F., Soliman, A. K., Sayed, G. A., & Saleh, K. R. (1998). Behavior and Ductility of Simple and Continuous Beams Reinforced with FRP Bars and Stirrups. ASCE Journal of Composites for Construction.
Bentz, E. C., Foster, S. J., Fernández Ruiz, M., Muttoni, A., Sigrist, V., & Walraven, J. C. (2010). Fédération Internationale du Béton (fib), Model Code 2010-First complete draft, chapters 7.3 and 7.13 (No. BOOK_CHAP). Fédération Internationale du Béton, Bulletin 56.
Reis, A. P. A. (1998). Reinforcement of reinforced concrete beams by means of additional steel bars or high-performance steel plates and mortar. Saint Charles. Dissertation (Masters)-School of Engineering of São Carlos-University of São Paulo.
Simões, M. L. D. F. (2007). Reforço à flexão de vigas de concreto armado por encamisamento parcial. Mestrado em Engenharia Civil, Universidade Federal do Rio de Janeiro (UFRJ), Rio de Janeiro/RJ, 162p.
American Concrete Institute - ACI 440. 2R-08. (2008). Guide for the design and construction of externally bonded FRP systems for strengthening concrete structures, Farmington Hills. MI-USA.
Fédération Internationale Du Béton - FIB. (2007). FRP reinforcement in RC structures, Technical Report, Bulletin 40, Switzerland.
Altun, F. (2004). An experimental study of the jacketed reinforced-concrete beams under bending. Construction and Building Materials, 18(8), 611-618.
De Janeiro, R. (2014). NBR 6118: projeto de estruturas de concreto–procedimento. Rio de Janeiro.
American Concrete Institute, ACI 318. (2011). Building Code Requirements for Structural Concrete and Commentary, Farmington Hills, MI USA.